Processing Guide:
|
PA 66 - Polyamide 66
|
 |
|
Extruder:
|
Single Screw Extruder Without vacuum, plain feeding section
|
 |
|
Screw Design:
|
Barrier Screw or Polyolefin Screw with equal feed ,transition and metering section, 25-30 L/D
Two mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section
|
 |
|
Compression Ratio:
|
3-4:1
|
 |
|
Cylinder Temperatures:
|
260-290 C 500-554 F
|
 |
|
Melt Temperature:
|
280-300 C 536-572 F
|
 |
|
Pre-Drying:
|
3 hours at 80 C (176 F) (very important)
|
 |
|
Calibration:
|
|
 |
|
Miscellaneous:
|
process above 250 oC (482 F) to avoid freeze-off if bubbles come then temperature too high increased output/reduced wear by preheating of material 75 C (167 F) or by heating of feeding section at 160 C (320 F)
|
|