Processing Guide:
|
PE-LD - Low-density polyethylene
|
 |
|
Extruder:
|
Single Screw Extruder with vacuum, grooved feeding section
|
 |
|
Screw Design:
|
Barrier Screw, 25-30 L/D
Two mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section
|
 |
|
Compression Ratio:
|
3,5:1
|
 |
|
Cylinder Temperatures:
|
170-200 C 338-392 F
|
 |
|
Melt Temperature:
|
180-210 C 356-410 F
|
 |
|
Pre-Drying:
|
No, 3 hours at 80 C (176 F) for regrind
|
 |
|
Calibration:
|
|
 |
|
Miscellaneous:
|
slip additivated PE-LD as blend partner gives 10-20% higher specific output Larger screw diameter : continuously two channels (improved conveying in feeding section)
|
|