Processing Guide:
|
PE-HD - High-density polyethylene
|
 |
|
Extruder:
|
Single Screw Extruder with vacuum, grooved feeding section
|
 |
|
Screw Design:
|
Barrier Screw, 25-30 L/D
Two mixing sections: dispersive-mixing spiral-shear element, rhomboid distributive-mixing section
|
 |
|
Compression Ratio:
|
3:1
|
 |
|
Cylinder Temperatures:
|
: 180-205 C 356-401 F
|
 |
|
Melt Temperature:
|
180-205 C 356-401 F
|
 |
|
Pre-Drying:
|
No, 3 hours at 105-110 C (221-230 F) for regrind
|
 |
|
Calibration:
|
|
 |
|
Miscellaneous:
|
bimodal PE-HD needs motor with 10-15% higher torque and has higher melt pressure/melt temperature Larger screw diameter : continuously two channels (improved conveying in feeding section)
|