Processing Guide:
|
ABS - Acrylonitrile-butadiene-styrene
|
 |
|
Extruder:
|
Single screw, no vacuum, grooved feeding section
|
 |
|
Screw Design:
|
Barrier screw 25 - 30 L/D
|
 |
|
Compression Ratio:
|
2,75 : 1
|
 |
|
Cylinder Temperatures:
|
190-240 C 374-464 F
|
 |
|
Melt Temperature:
|
200-245 C 392-473 F
|
 |
|
Pre-Drying:
|
3 hours at 70-80 C (158-176 F)
|
 |
|
Calibration:
|
|
 |
|
Miscellaneous:
|
approx. 30 % higher torque (than PVC)
|
|